Rolling Direction in Non-Oriented Electrical Steel: When It Matters for Stator and Rotor Design

Rolling Direction in Non-Oriented Electrical Steel: When It Matters for Stator and Rotor Design

Rolling Direction in Non-Oriented Electrical Steel: When It Matters for Stator and Rotor Design

Electrical steel laminations stacked with rotational offset so the rolling direction varies around the stator core

Rolling direction in electrical steel still matters when the grade is sold as non-oriented. The catalog core loss of a non-oriented (NO) grade is measured on an Epstein specimen made of half rolling-direction (RD) and half transverse (TD) strips, so the datasheet value is a mixed-direction figure. IEC 60404-8-4 allows 0.35 mm and 0.50 mm fully processed grades a loss anisotropy of ±8% to ±17%, depending on grade. For a full-ring stator that average is usually adequate. For segmented teeth, linear cores, rotor bridges near their limit and low-cogging designs, it may not be.

Why non-oriented electrical steel is not fully isotropic

Cold-rolled electrical steel coils; rolling direction is set at the mill

NO steel is engineered to minimize in-plane anisotropy, not to eliminate it. JFE Steel describes its NO products as polycrystals “designed so as to minimize magnetic anisotropy in the steel sheet plane” (JFE Technical Report No. 6). Cold rolling leaves a crystallographic texture, and that texture makes RD and TD behave differently in magnetic and, to a smaller degree, mechanical properties. IEC 60404-8-4 sets a maximum anisotropy of loss for every grade, a limit that only makes sense because the two directions are expected to differ. The practical question for electric motor stator and rotor design is not whether anisotropy exists, but whether the core geometry averages it out or locks it in.

What does the datasheet core loss represent?

Steel strip being slit along the rolling direction

The headline W15/50 value (specific total loss at 1.5 T, 50 Hz) on an NO datasheet is normally an Epstein result on a mixed specimen. Under IEC 60404-2 and ASTM A343/A343M, a mixed specimen has half its strips cut parallel and half perpendicular to the rolling direction, with the parallel strips in two opposite branches of the frame and the perpendicular strips in the other two. ASTM A1036 notes that this half-and-half specimen is normally used for NO grades under ASTM A677, and defines the “50-50 Epstein equivalent” loss as the arithmetic mean of the parallel and transverse values. Mill catalogs say the same: JFE’s N-CORE and Nippon Steel’s NO tables are measured on as-sheared specimens cut half along and half across the rolling direction (JIS C 2550).

IEC 60404-8-4 also gives the buyer two levers that most drawings never use. Clause 7.1.3 allows a loss requirement on parallel-only or perpendicular-only strips to be agreed at enquiry and order. Clause 7.1.4 allows the buyer to require declaration of the measured anisotropy of loss, not just conformance to the maximum.

How large is non-oriented electrical steel anisotropy?

The maximum anisotropy of loss in IEC 60404-8-4 (edition 4.1, 2026) depends on the grade:

IEC 60404-8-4 grades (fully processed)Nominal thicknessMax. specific total loss at 1.5 T, 50 Hz (W/kg)Max. anisotropy of loss at 1.5 T
M210-35A5 to M360-35A50.35 mm2.10 to 3.60±17%
M230-50A5 to M290-50A50.50 mm2.30 to 2.90±17%
M310-50A5, M330-50A50.50 mm3.10, 3.30±14%
M350-50A5, M400-50A50.50 mm3.50, 4.00±12%
M470-50A5 to M800-50A50.50 mm4.70 to 8.00±10%
M940-50A5, M1000-50A50.50 mm9.40, 10.00±8%

Source: IEC 60404-8-4:2022+AMD1:2026, Table 1. Magnetic properties measured by the Epstein method per IEC 60404-2. The same table allows ±6% to ±15% for 0.65 mm and 1.00 mm grades; Table 2 (0.47 mm, 60 Hz grades) allows up to ±18%.

Two points matter for design. The low-loss, high-silicon grades that motor designers prefer carry the widest permitted anisotropy, not the narrowest. And the standard limits anisotropy of loss only; Table 1 has no corresponding anisotropy limit for polarization (B50 at H = 5,000 A/m).

Anisotropy of loss is commonly defined as T = (PTD − PRD) / (PTD + PRD) × 100%. Taking the mixed Epstein value as the mean of the two directions, as ASTM A1036 does, a grade at the ±17% limit could have a transverse-only loss up to 17% above the mixed value and a rolling-direction loss up to 17% below it. Real coils are usually inside the limit; Tata Steel’s typical data sheet for SURA M270-35A lists an anisotropy of loss of 10%. The drawing, however, tells you nothing about where your coil sits inside the band.

Where does rolling direction in electrical steel change the design?

The table sorts common core features by whether the geometry averages RD and TD or fixes one orientation. What to specify for each is collected in the drawing and RFQ checklist further down.

Core featureDoes the geometry average RD and TD?What the mixed datasheet value can hide
One-piece ring statorGlobally yes: teeth point in every direction around the circumferenceLocal loss and flux differ tooth to tooth; possible extra cogging harmonics in low-cogging designs
Segmented teeth (T-segments, pole-chain)No: every tooth has the same orientation to RDTooth loss and permeability follow one direction, not the average
Linear or straight-segment coresNoSame as segmented teeth, plus yoke flux in one fixed direction
IPM rotor bridges and ribsPartly: bridges sit at many angles to RD, but each bridge’s angle is fixed within a laminationYield strength differs slightly by direction, and which direction is weaker depends on the grade
Rotational (rotary) stackingDistributes orientation and thickness variation around the stackCan change cogging harmonics; not automatically beneficial
Wire EDM prototypeDepends on how the part was placed on the sheetPrototype orientation may not match the production strip layout

One-piece ring stators: the average holds globally, not locally

Stator lamination stamped from non-oriented electrical steel

In a full ring, the teeth sweep through every angle to the rolling direction, so the total core loss tends toward the mixed-direction figure. The loss distribution does not. In a Cardiff University PhD study (Somkun, 2010), an induction motor model core built from 0.50 mm NO steel showed localized loss in the stator teeth, tooth roots and back iron that differed from the average value by 52%, 19% and 36% respectively, which the author attributed to magnetic anisotropy. For most ring stators this is a second-order effect on total loss, but a model built on mixed data can match total loss and still miss local hot spots or vibration behavior.

Cogging is the other exception. Kim et al. (Mathematics, 2026) studied an 8-pole, 12-slot surface PM motor with a 50PN470 core. Anisotropy interacted with slot harmonics to produce a distinct 16th-order cogging harmonic, and both 3D FEA and prototype measurements showed it persisting after conventional step-skewing. Their model assumed a transverse saturation flux density only 2% lower than RD, which shows how small a material difference can produce a measurable harmonic.

Segmented teeth and linear cores: the average no longer applies

Once each tooth is punched as a separate segment, every tooth has the same orientation to the rolling direction. Tooth flux is mainly radial, and JFE’s local measurements in model motors found flux density and iron loss highest in the teeth, so the tooth now behaves like RD or TD material, not the 50/50 average.

Rens et al. (ArcelorMittal Global R&D, World Electric Vehicle Journal, 2016) modeled a segmented IPM stator and found that applying RD material data to the teeth, while keeping mixed data in the yoke, significantly improved the predicted results. Segmentation had an overall positive effect if the parasitic airgap could be ignored; with a 50 µm airgap between segments, torque was still nearly 2% lower than the unsegmented machine, although efficiency improved. Soda, Hayashi and Enokizono (IEEE Transactions on Industry Applications, 2021) likewise treated rolling direction as a design variable for segmented SPM stator cores. JFE has even developed a grain-oriented grade, JGE, specifically for segmented motor cores (JFE Technical Report No. 4). That is outside the NO family, but it shows the direction of travel: in segmented cores, orientation is a design parameter.

FEA material model: mixed curve or direction-specific data?

Most motor models use one isotropic B-H curve and one loss curve, usually derived from mixed Epstein data. That is defensible for a ring stator. For segmented cores it builds the wrong material into the teeth. Two practical upgrades exist:

  1. Direction-specific data. Ask the mill for RD-only and TD-only Epstein or single-sheet results for the grade and thickness you will buy, through the clause 7.1.3 agreement described above. ASTM A1036 describes single-sheet testing in each direction.
  2. Anisotropic material models. Commercial FEA codes support orthotropic B-H definitions (Kim et al. used an orthotropic model in JMAG), and research codes use vector models such as the Enokizono and Soda model. Assign RD data to segment teeth and keep mixed data only where the geometry genuinely averages.

Either way, calibrate the model against a stack measurement. Datasheet values, mixed or directional, describe strips, not a punched, joined core; see our discussion of why FEA core loss and finished-product loss diverge and how stacking factor differs between datasheet and built core.

Rotor bridges: mechanical properties by direction

Bridge sizing in an IPM rotor balances leakage flux against stress at overspeed, as covered in our rotor bridge design guide. Yield strength enters that check directly, and it depends on direction. JFE publishes typical tensile data for both directions, measured on as-sheared JIS No. 13A specimens per JIS Z 2241 (typical values, not guarantees):

JFE gradeThicknessYield point L / C (N/mm²)Tensile strength L / C (N/mm²)Lower yield direction
35JN2500.35 mm405 / 417531 / 546L (rolling)
35JNE2500.35 mm349 / 351468 / 482L (rolling)
35JNE4400.35 mm296 / 291415 / 399C (transverse)
20JNEH12000.20 mm375 / 388496 / 515L (rolling)

Source: JFE Steel, Electrical Steel Sheets catalog (f1e-001), N-CORE typical mechanical properties. “L” and “C” are specimens cut parallel and transverse to the rolling direction.

The directional difference in these grades is a few percent, smaller than typical uncertainty from cut-edge condition or stress-relief annealing, so it rarely decides a design by itself. But the sign is not consistent: three of these grades are weaker in the rolling direction and one is weaker in the transverse direction. For a bridge designed close to its limit, use the lower of the two published values for the grade you will actually buy, and state the delivery condition, rather than a single catalog number. The rotor design pillar covers the wider material selection.

Rotational stacking: averaging tool or harmonic source?

Rotational stacking means rotating laminations, or groups of laminations, by a fixed angle as they are stacked. Its established manufacturing purpose is thickness compensation. A progressive-die patent from L. H. Carbide (US 5,359,763) describes half-turn reversals of the stack “to compensate for nonuniform strip thickness to obtain a rotor or stator of substantially uniform height,” triggered by gauged cross-feed thickness differential, and China Steel Corporation’s 2024 stacking-system paper uses jig rotation for the same reason.

Rotation also redistributes orientation to RD around the stack, and the literature does not agree that this is always helpful. Yamaguchi, Daikoku and Takahashi (COMPEL, 2004) found that PM motors with parallel-laminated and rotationally laminated cores show different cogging torque waveforms because of anisotropy. Kim et al. (2026) went further and recommended “reducing the implementation of rotational stacking of stator laminations” to mitigate the anisotropy-induced cogging harmonic in their motor. Rotational stacking should therefore be a deliberate, analyzed choice, written on the drawing as required, prohibited or supplier’s option, with the angle stated.

Does a Wire EDM prototype represent the production core?

Wire EDM cutting a toothed part, as used for prototype laminations

Only if it was cut in the same orientation. A Wire EDM prototype can be placed anywhere on a sheet at any angle, and the operator will often nest it for material use or convenience. In simple-die and progressive-die stamping, every blank’s orientation to the rolling direction is set by the strip layout and does not change from part to part.

Stamping presses for progressive-die lamination production

For a one-piece ring this rarely matters. For segments it matters a lot. If prototype segments were cut with tooth axes along RD and the production strip layout nests them across the strip to improve material utilization, the production teeth see TD properties that the prototype test never measured. The same applies to rotor laminations where a critical bridge lands at a different angle to RD. Wire EDM and stamping also leave different cut-edge conditions, so a prototype test confounds two variables if orientation is not controlled.

What should appear on the lamination drawing and RFQ?

  • Orientation: for segmented, linear or bridge-critical parts, an arrow or note fixing the part axis relative to the rolling direction, with a tolerance if it matters.
  • Material data basis: whether FEA used mixed Epstein data or direction-specific data, and which test standard and condition (for example, W15/50 per IEC 60404-2).
  • Anisotropy: whether the measured anisotropy of loss must be declared on the mill certificate (IEC 60404-8-4, 7.1.4), or whether a parallel-only or perpendicular-only loss requirement applies (7.1.3).
  • Mechanical basis: for rotor bridges, which direction’s yield value the stress check used and in what delivery condition.
  • Stacking: rotational stacking required, prohibited or supplier’s option; angle if required.
  • Prototype traveler: the orientation in which Wire EDM prototypes were cut, so production can match it or the difference can be assessed.

How we approach it at Yucore Technologies

Our process path runs from Wire EDM prototypes through simple-die and progressive-die stamping, in lamination thicknesses from 0.15 mm to 0.5 mm. Rolling direction is one of the few design inputs that changes silently between those stages: the prototype operator chooses it, and the production strip layout fixes it. We therefore ask about part orientation at the prototype stage for segmented and bridge-critical laminations, so the prototype is cut the way the production die will present the strip. Where a design needs direction-specific material data, the request belongs in the steel order, before the coil is bought. If your design is sensitive to orientation or stacking, send us the drawing and we will review it against the intended strip layout.

Frequently asked questions

Is non-oriented electrical steel isotropic?

Not fully. It is designed to minimize in-plane anisotropy, but rolling leaves a texture that makes rolling-direction and transverse properties differ. For 0.35 mm and 0.50 mm grades, IEC 60404-8-4 limits the anisotropy of loss at 1.5 T to between ±8% and ±17% depending on grade, with the low-loss 0.35 mm grades allowed ±17%.

Is the datasheet W15/50 value measured in the rolling direction?

Normally not. Epstein specimens for NO steel are normally half parallel and half perpendicular to rolling, and mills such as JFE and Nippon Steel state the same in their catalogs. The datasheet value is a mixed-direction figure.

When should rolling direction be on the lamination drawing?

When the geometry does not average the two directions: segmented teeth, linear cores and rotor laminations with a bridge designed close to its limit. For a one-piece ring stator it is usually unnecessary, except in cogging-sensitive designs where anisotropy has been shown to create extra harmonics.

Sources

  • IEC 60404-8-4:2022+AMD1:2026 CSV, Table 1 and clauses 7.1.3, 7.1.4.
  • IEC 60404-2:1996+AMD1:2008, Epstein frame method.
  • ASTM A343/A343M-14(2019); ASTM A1036-04(2009), Annex A2.
  • JFE Steel, Electrical Steel Sheets catalog f1e-001; JFE Technical Report No. 4 (2004) and No. 6 (2005).
  • Nippon Steel, Non-Oriented Electrical Steel Sheets catalog D005je.
  • Tata Steel, SURA M270-35A typical data sheet.
  • S. Somkun, PhD thesis, Cardiff University, 2010.
  • J. Rens et al., World Electric Vehicle Journal 8(2), 2016, doi:10.3390/wevj8020450.
  • N. Soda, N. Hayashi, M. Enokizono, IEEE Trans. Ind. Appl. 57, 2021, doi:10.1109/TIA.2021.3091947.
  • J.-H. Kim et al., Mathematics 14(4), 650, 2026, doi:10.3390/math14040650.
  • S. Yamaguchi, A. Daikoku, N. Takahashi, COMPEL 23(3), 2004, doi:10.1108/03321640410540548.
  • US Patent 5,359,763 (L. H. Carbide Corporation, 1994); China Steel Technical Report No. 37 (2024), pp. 79 to 82.